2026-11-05 · 5 min read

Two tungsten electrodes sit side by side on a bench. One has a red band, one has a grey band. That's the whole difference most buyers can see, and it's enough to tell them apart. It's not enough to pick one.

Here's the short version. Red is thoriated: 2% thorium oxide. Grey is ceriated: 2% cerium oxide. Both are 2% electrodes, both are tungsten, both weld. The band tells you which classification you're holding. It doesn't tell you whether that's the right one for the job, and it says almost nothing about the rod itself.

What the band actually encodes

The colour labels a classification, and that classification is written in two standards that don't use the same codes.

  • Thoriated, 2%: ISO 6848 WT20, AWS A5.12 EWTh-2
  • Ceriated, 2%: ISO 6848 WC20, AWS A5.12 EWCe-2

Don't mix the two systems on one purchase order line. WT20 and EWTh-2 are the same electrode described in two vocabularies. Same for WC20 and EWCe-2. Write one system or write both, but don't write WT20 beside EWCe-2 and expect the supplier to sort it out.

Behind each code sits an oxide range. Thoriated runs 1.7–2.2% thorium oxide. Ceriated runs 1.8–2.2% cerium oxide. That's what "2%" means in practice: a nominal figure with tolerance either side, not a fixed number stamped into every rod.

The band does not measure the rod

Three things colour can't tell you.

  • Where inside the range the oxide actually sits. A rod at 1.7% and a rod at 2.2% carry the same band.
  • Whether the diameter and length in your hand are what the box says.
  • Whether the surface is clean and straight, or bent enough to make the tip wander.

That last one hurts more than the band helps on thin-section work. So read the label after the band: classification, diameter, length, quantity. If the band and the label disagree, the label wins — and you should ask us about it.

One wrinkle worth knowing. Ceriated used to ship with an orange band. Grey is the colour now, but orange still turns up on old wall charts, old stock, and drawings nobody has updated since. If you're matching electrodes to a weld procedure written years ago, check whether the colour in it is still the colour in use.

The difference that changes your day

Thoria is radioactive. Ceria is not. That single line is why ceriated went from specialty item to default in a lot of shops, and it's why the choice is often made by whoever handles the grinding dust rather than whoever sets the amps.

If you grind tungsten, the dust is your exposure route — not the rod sitting in its box. Storage, grinding and disposal tend to be governed by local rules rather than by an electrode catalogue, so check yours before you standardise a shop on thoriated stock. If nothing on your work forces you to keep thoria, ceriated costs you nothing in welding terms and removes the question.

Power source and current range

This is where the two stop being interchangeable.

  • WT20 runs on DC, normally from a transformer-type constant-current supply. It starts well, burns off at a medium rate, and sits in the middle of the current range.
  • WC20 runs on AC or DC, on an inverter or a transformer. It restrikes better, lasts longer, is strongest at low current, burns off slowly, and doesn't spit.

Read that as a selection order, not a ranking. Thin sheet at low amps, or anything that needs AC: ceriated is the one that behaves. Medium current on DC over heavier work: thoriated starts well and does the job, provided you're set up to handle it.

The failure mode is worth naming. An electrode run past the current its tip was prepared for doesn't fail politely. It erodes, the arc wanders, and the weld goes with it. Match the tip to the amps, not the band to the machine.

If you're switching over

Treat it as a procedure change, not a stock swap. Same amps with a different classification is not the same weld, even when both rods are nominally 2%. Run a test piece on the section you actually weld, look at the arc start and the bead, and adjust from there.

Two habits make the switch boring, which is what you want.

  • Keep one classification per bin. Mixed bins are how a red rod ends up in a grey box.
  • Write the classification on the job card, not the colour. Colours change. WT20 and WC20 don't.

What to put on the order

Four lines and there's nothing left to guess.

  • Classification: WT20 or EWTh-2, WC20 or EWCe-2
  • Diameter and length
  • Quantity
  • Whether the batch needs a certificate

Our ceriated stock ships 10 pieces to a plastic box, minimum 50 pieces. Thoriated ships 10 to a plastic box as well, minimum 200 pieces. Both product pages carry the standard, so the page, the box and your PO can be made to agree before anything ships.

Pick in one line

Red band, thoriated: radioactive, DC, medium current, starts well. Grey band, ceriated: not radioactive, AC or DC, strongest at low current, longer life. Both nominally 2%. Both tungsten.

The band gets you the classification in one glance. Everything after that — the oxide range, the diameter, the certificate, whether thoria is allowed in your shop — comes off the label, off your procedure, and off your local rules.

Selection guidance only. The standard and the manufacturer's technical data govern; confirm the numbers on the quote before you commit a batch.