2026-11-04 · 5 min read

E308-16 and E308L-16 weld the same family of 18-8 austenitic stainless steel. They share a rutile coating, they both run on AC or DC, and they both sit in AWS A5.4. A buyer comparing the two on a data sheet sees almost identical numbers. The one that differs is carbon, and it is the reason both exist.

The carbon limit

E308-16E308L-16
StandardAWS A5.4AWS A5.4
Deposited carbonStandard limit for the gradeHeld to a maximum of 0.03%
Usable currentAC or DCAC or DC
CoatingRutileRutile
CostLowerHigher

The L stands for low carbon. Holding the deposit to 0.03% and below is the entire purpose of the grade, and it is worth understanding why a few hundredths of a percent matters enough to justify a separate designation.

Why carbon is the problem in stainless

In an austenitic stainless steel, carbon and chromium combine. Given enough carbon and enough time in the temperature range where the atoms can move, chromium carbides form at the grain boundaries. That removes chromium from the metal immediately around each boundary, and chromium is the element that makes the steel stainless in the first place. The result is a narrow band along the grain boundaries that is no longer resistant, and corrosion starts there while the rest of the plate is untouched.

That temperature range is reached routinely during welding, in the heat-affected zone and in the deposit. If the finished part can be solution annealed afterwards — heated enough to dissolve the carbides and quenched — the carbon content stops mattering. Most fabricated parts cannot be, or the customer will not pay for it. That is the situation the L grade was created for.

When the plain grade is the right choice

E308-16 is not the inferior option. Where the joint will not see a corrosive environment, or where the assembly is annealed afterwards, the standard carbon grade welds perfectly well and costs less. Specifying E308L for a guard rail is not wrong, it is just paying for a property the job does not use.

The opposite mistake is more expensive. Using E308-16 on a vessel that will hold a chloride-bearing liquid, or on a part that will be in service for a decade, is choosing to put a chromium-depleted band into the one place corrosion will find first.

The same logic runs through the wire range

This is not a stick-electrode distinction. The same L appears in ER308L and ER316L, and for the same reason. Our stainless wire line carries ER308 and ER308L as separate designations, and the four-grade TIG filler line includes ER308L rather than ER308 — because the jobs that buy straight TIG filler, pressure vessels and process pipework, are exactly the jobs where the carbon limit matters.

One thing the L does not do

It does not make a 308 filler suitable for 316 base metal. The molybdenum that gives 316 its resistance is not in either grade. If the plate is 316, the filler is E316L-16 or ER316L, and the carbon question is secondary. Matching the alloy family comes first; the L is the refinement after that.

Both grades are supplied to AWS A5.4 and both can be ordered with the certificate for the standard. Tell us the base metal and what the part will be exposed to, and the choice between them becomes obvious.