2026-11-04 · 6 min read
Filler selection starts with the base metal, not with the process and not with what is already on the shelf. The reason is mechanical rather than administrative: the deposit and the plate have to end up with comparable strength, comparable corrosion behaviour and, in stainless work, a comparable structure. Pick the filler first and the joint decides for you later.
The common pairs
| Base metal | Stick | Wire | Note |
|---|---|---|---|
| Mild and low-carbon steel | E6013, E6011, E7018 | ER70S-6, E71T-1C, E71T-GS | E6013 for general work; E7018 where the joint is restrained or the code calls for low hydrogen |
| Low-alloy Cr-Mo steel | E8018-B2 | ER55-B2, ER55-B2MnV | The Cr and Mo in the filler match the creep-resistant base metal, not the strength figure |
| 9Cr-1Mo-V (P91 / T91) | Matching 9Cr electrode | ER90S-B9 | Do not substitute a carbon steel filler; the creep behaviour is the whole point of the base metal |
| 304 / 18-8 austenitic stainless | E308-16, E308L-16 | ER308, ER308L | Use the L grade where the joint sees corrosive service or cannot be annealed afterwards |
| 316 / 316L stainless | E316L-16 | ER316L | The molybdenum is in the filler because it is in the plate. E308L is not a substitute |
| Duplex stainless | — | ER2209 | Duplex filler for duplex plate; the ferrite balance is the reason |
| Carbon steel to stainless (dissimilar) | E309 type | ER309L | The higher chromium lets the dilution land in a structure that tolerates it |
| Aluminium and its alloys | E4043 | Aluminium brazing wire, 419 °C or 505 °C | Fusion welding or brazing, depending on section and alloy |
| Copper to aluminium | — | Cu-Al flux-cored brazing wire | These two cannot be fusion welded to each other without brittle intermetallics |
| Copper, brass, copper alloys to steel | — | HL301 silver brazing rod | Brazing, so the base metal is not melted |
| Tool steel (P20, H13, SKD61, SKD11) | — | P20, SKD61 / SKD11 / H13 wire | Match the base metal being repaired; a mismatched filler is the usual reason a tool repair fails |
| Surfacing and hardfacing | ECoCR-E | ERCoCr-C | A deposit chosen for wear behaviour, not for joint strength |
Cast iron is the honest gap
Cast iron is not in the table above because we do not supply a filler for it. Cast iron is normally joined with nickel or nickel-iron electrodes, or brazed, and we do not stock either. If a job calls for it, say so and we will tell you rather than sell you a mild steel electrode that will crack at the fusion line.
Three pairs people get wrong
- 316 plate with a 308 filler. It welds and it looks right. The molybdenum that makes 316 resistant to chlorides is missing from the deposit, so the weld becomes the least resistant part of the assembly.
- Dissimilar carbon-to-stainless with a carbon steel filler. The deposit picks up chromium and nickel by dilution and can harden enough to crack. A 309 type filler exists for exactly this.
- Low-alloy Cr-Mo plate with a high-strength carbon steel filler. The tensile figure may match and the creep behaviour will not, which is what the Cr and Mo were there for.
One more thing worth stating plainly: matching the base metal is the first filter, not the last. Service temperature, position, thickness and the code the job is built to all narrow the choice further. Send the base metal specification and the service condition and we will name the grade rather than the family.