2026-11-04 · 6 min read
E7015, E7016 and E7018 all deposit a minimum of 70,000 psi tensile strength and all three carry a hydrogen-controlled coating. On a quotation they differ by one digit. On the job they differ by which machine can run them and how fast they fill a joint.
The last digit is the whole difference
| Designation | Coating | Current | Positions | Deposition |
|---|---|---|---|---|
| E7015 | Low hydrogen, sodium type | DC only | All | Standard for the coating |
| E7016 | Low hydrogen, potassium type | AC or DC | All | Standard for the coating |
| E7018 | Low hydrogen with iron powder added | AC or DC | All | Higher, because the iron powder becomes part of the deposit |
In the AWS numbering, the fourth digit states coating and current together. A 5 means a low-hydrogen coating intended for direct current. A 6 means a low-hydrogen coating that will also strike and hold an arc on alternating current. An 8 means the same DC-or-AC usability with iron powder in the coating.
That is why the AC-versus-DC question decides more purchases than the strength figure does. If the only machine on site is a DC set, all three work. If it is an AC transformer, E7015 is out.
Why the potassium matters
The difference between E7015 and E7016 is the binder in the coating. The sodium type needs direct current to establish and hold the arc; the potassium type will re-strike on alternating current, because the potassium compounds are there to stabilise the arc through the zero crossing that AC goes through every half cycle. This is a real constraint, not a preference.
The practical consequence is on restarts. An E7016 restarts more easily than an E7015, which is one of the reasons it appears on pipe work and on structural joints where the operator is stopping and starting at the end of every rod.
Where E7018 earns its place
The iron powder in an E7018 coating is not an additive to the metallurgy, it is bulk that becomes deposit. More metal goes into the joint per arc-hour, and the arc is smoother because the coating melts in a steadier way. On structural fabrication and on long fillets, that is the difference between finishing the day and finishing the week.
The cost is on the other side of the ledger. A heavier coating means more to keep dry, and a low-hydrogen electrode that has absorbed moisture no longer does the job it was bought for. If the rods sit open on a bench overnight, the advantage of the coating is gone and the joint would have been better served by a rutile electrode than by a damp low-hydrogen one.
A note on storage
All three are hydrogen-controlled, and hydrogen control only works if the electrode is dry when it is used. Keep them in a sealed container or a holding oven, and re-dry according to the temperature stated on that grade’s datasheet rather than a figure remembered from another product. We do not print drying temperatures in this guide because they differ between coatings, and quoting one here would invite it to be applied to the wrong electrode.
The short version
- Only a DC machine available, and the job is restrained or code-governed: E7015.
- AC or DC, all-position pipe or structural work where the operator restarts often: E7016.
- AC or DC, structural fabrication, fillets and fill passes where deposition rate is the cost driver: E7018.
All three are supplied against the AWS A5.1 classification. Tell us the machine and the joint and we will name the one we would run.